Most of the questions we get about explosion clad pipe come in two flavours. Procurement asks whether the bond can be trusted. Engineers ask what actually happens between the clad plate leaving the bonding site and the pipe arriving on a project yard. This note answers both from three documents we use every day: our clad plate technical requirements, the mill’s processing workflow card, and API Spec 5LD. Every number below comes straight from them.
If you need the wider picture first, covering clad, lined and overlay pipe and how the three compare, our Cladding Pipe Guide is the better starting point. This one covers a single route, plate to pipe.
API 5LD defines clad pipe as a bimetallic pipe whose CRA layer is metallurgically bonded to the backing steel. It lists the accepted ways of getting there: hot rolling, coextrusion, weld overlay, explosion bonding, powder metallurgy, or another process that produces a metallurgical bond. For welded clad pipe, the standard says it is produced from plate or skelp clad by one of those processes, and the backing material has to meet API 5L PSL 2. Unless agreed otherwise, the CRA layer must be at least 2.5 mm thick.
Explosion bonding earns its place on that list because the joint forms in microseconds. The detonation drives the cladding plate into the base plate at high speed, and the oblique impact throws a jet of surface metal ahead of the collision point. That jet strips away oxides and contamination, leaving clean metal to meet clean metal. The result is the wavy interface seen on every macro section. With no fusion, the CRA chemistry is not diluted by the carbon steel, unlike an overlay-welded bore.
For an SS316/316L explosion bonded clad pipe order, the plate is specified as S31603 + carbon steel. The production standard is NB/T 47002.1-2019 Class B1, with base material to GB/T 713.2-2023 and cladding to GB/T 713.7-2023. Clad and base thickness follow the RFQ; where the RFQ is silent, the base, cladding and total thickness all take the default negative tolerance. Plate made this way is also sold on its own through our explosion bonded clad plates line.
Before lay-up, the bonding face of the base plate is ground to Ra ≤ 12.5 μm while holding the required plate thickness. It must be free of mill scale, pitting and depressions, and mill scale on the non-bonding faces is removed completely. The cladding is ground too: an 80-grit wheel for roughing, a 120-grit wheel for finishing, always running along the long edge. In transfer the clad face stays under cardboard, and steel stamps go only in the scrap allowance. Base cutting must keep the layout lines, with cut-face unevenness under 5 mm. Cladding flatness is held to ≤ 5 mm/m, and ≤ 10 mm across the whole sheet. Where the cladding has to be made from more than one sheet, the splice welds get 100% PT to NB/T 47013-2015 Level I.
After the shot, the whole plate goes through 100% UT to NB/T 47013.3-2023, and the result has to meet NB/T 47002.1-2019 Class B1. Any unbonded area is handled by the specified repair welding procedure. The plate is then heat treated and the substrate face is cleaned with an oxy-acetylene torch until no mill scale remains. Leveling brings flatness to ≤ 7 mm/m and ≤ 10 mm/2 m. For wave spacings between 300 mm and 1000 mm, the deviation may not exceed 1.0% of that spacing.
Test coupons are cut by plasma, with the cladding protected while they are taken. A second full UT then confirms the bonding rate still meets Class B1 after leveling. Flattening can open marginal bond areas that passed the first scan. Repair welds on the cladding receive 100% PT to NB/T 47013.5-2015 Level I and are belt-ground to Ra ≤ 6.3 μm. Final layout allows a 15 mm trim margin. The cladding face is marked with felt-tip pen only, never die stamps, and transferred marks sit in the scrap zone as low-stress stamps. The last step is pickling and passivation, after which the CRA surface has to be free of oxide scale and over-pickling.
Mill-level plate acceptance is only half the story. API 5LD clause 11.1.2 requires clad plate for welded clad pipe to be ultrasonically inspected before forming to ASTM A578-07. Scanning follows a continuous grid on 1 in. centers, and acceptance is Level C. Disbonding counts as a defect. It is not permitted within 50 mm of any edge to be longitudinally welded, or within 100 mm of any pipe end (12.2.4). For bond strength, clause 8.3 calls for a bond shear test on one pipe in every 50, with a minimum of 137.8 MPa (20,000 psi). By agreement, a flattening test can replace it. Good explosion bonds test well above that floor. The contract figure should still be the one the standard and the PO state.
The pipe side of the process runs on a workflow card that doubles as the quality tracking record. Each operation carries a TPI hold, witness or review point. The card quoted here comes from a recent Φ457 mm order in ASTM A671 CC65 + UNS N08825, built to API Spec 5LD for a Middle East sour-gas EPC project, with Alloy 625 used for the seam cladding and end overlays. That combination is our Incoloy 825 clad line pipe route. An SS316L clad pipe follows the same sequence with its own qualified WPS and acceptance values.
Heat treatment and sizing follow. On the Φ457 order, body OD was held to ± 3.2 mm, end ID to Φ428.74 ± 1.0 mm and end out-of-roundness to ≤ 3.0 mm.
The pipe end is where clad pipe most often fails in the field, usually because girth welding meets a bond line. The Alloy 825 cladding within 110 mm of each end is machined off to 0.5 mm below the bonding interface. A copper sulfate test to ASTM A967/A967M Practice D proves the alloy is fully gone, and remaining base wall may not drop below 87.5% of nominal. The area is then polished to Ra ≤ 0.2 μm, cleaned and overlay-welded to 4.5 (0, +2.0) mm, with one test piece for every 20 pipes.
After straightening, PMI checks the overlay against Cr 20–23%, Mo 8–10%, Ni ≥ 58%, Cb 3.15–4.15% and Fe ≤ 10%. Each end is faced by at least 7 mm to remove the UT dead zone. The finished bevel is 37.5° ± 2.5° with a 1.6 ± 0.8 mm root face, and overlay thickness at the end must stay ≥ 3.5 mm. This is the same thinking behind our weld overlay pipes, applied only where it is needed.
The seam gets 100% UT to ASME Section V Article 4. The pipe body is ultrasonically scanned to ISO 10893-8 and ASTM A578, with no recordable defects allowed within 100 mm of the end or 50 mm of the seam bevel. Hydrostatic test pressure is calculated from P = 2St/D at S ≥ 60% SMYS, which gave 7.0 MPa on this order. It is held for at least 20 s, with test water at ≤ 30 ppm chloride. The whole bore is then PT-inspected and pickled and passivated to ASTM A380, again with water at ≤ 30 ppm chloride. Residual magnetism must not exceed 15 GS. Hardness is taken at no fewer than five points each in the carbon steel HAZ and the CRA, with limits of ≤ 248 HV10 and ≤ 335 HV10. The outside is blasted to Sa2.5, primed to ≥ 25 μm DFT and stencil-marked.
A pipeline is not just straight runs. The same explosion clad pipe serves as mother pipe for clad induction bends. These follow a 15-step route: incoming inspection, cutting, surface pre-treatment, medium-frequency bending and tempering, then machining, gauging, hydrotest, NDT and mechanical tests. Tees, reducers and elbows come from our clad pipe fittings shop, and clad flanges complete the package. For a side-by-side view, see our CRA clad pipe overview or the explosion welding pipe product page.
| Route | Bond type | Where it fits best |
|---|---|---|
| Explosion bonded clad pipe | Metallurgical, solid state | Large OD, heavy wall, sour service, risers and bends |
| Weld overlay pipe | Metallurgical, fusion | Short spools, fittings, small bores, pipe ends |
| Lined pipe | Mechanical | Long onshore flowlines where cost per metre leads |
We control the full chain: plate specification, bonding acceptance, forming, welding, end treatment and final testing. Each pipe traces back to its plate heat batch on one TPI-signed card. Send us the OD, backing grade, CRA grade and thickness, length, and the governing standard (API 5LD, DNV or a project specification). We will return a matched plate and pipe ITP before any steel is cut.
Yes. API 5LD names explosion bonding as one of the processes that produce a metallurgically bonded clad pipe, provided the backing steel meets API 5L PSL 2 and all test and inspection clauses are met.
API 5LD clause 8.3 sets 137.8 MPa (20,000 psi), tested on one pipe per 50. A flattening test may be substituted by agreement.
API 5LD sets a 2.5 mm minimum unless agreed otherwise. Common clad pipe orders use 3 mm, as on the Φ457 × (11.13 + 3) mm order described above.
Girth welds should not cross a bond line. Machining the cladding off 110 mm back and overlaying with Alloy 625 gives the field welder a homogeneous, fully fused CRA bore to weld on.
Through two full UT scans at the plate stage, before and after leveling, and then a UT per API 5LD 11.1.2 to ASTM A578 Level C. UT is repeated after forming at the seam zone and the pipe ends.
Yes. Clad bends are induction bent from the same mother pipe, and clad fittings and flanges use matching CRA grades