Mechanically Lined Pipe (MLP) vs. Metallurgically Clad Pipe: Manufacturing, Testing, and Procurement Differences

When two bimetallic pipe offers sit side by side on a bid tabulation, the comparison usually stops at price per tonne and delivery date. Yet the real difference between a mechanically lined pipe and a metallurgically clad pipe is decided much earlier: on the mill floor, in the inspection and test plan, and in the paragraphs of the purchase specification that nobody reads until something goes wrong. This article looks at both products the way a QA engineer or a procurement lead sees them. It covers how each one is made, what is actually tested, which design rules apply, and what belongs in the RFQ. For a broader introduction to CRA layers and alloys, our Cladding Pipe Guide is a good place to start.

Mechanically lined pipe starts as two separate products. The outer pipe is a standard carbon steel line pipe, seamless or welded, whose bore is cleaned and blasted. The liner is a thin CRA tube, normally formed from strip and seam-welded, then inspected along its own weld. The liner is pushed into the outer pipe, and the assembly is expanded from the inside, either with water pressure or with a mechanical expander drawn through the bore. The liner yields; the outer pipe is strained only elastically. When the load is removed, the outer pipe tries to recover its original size and clamps the liner. The pipe ends are then trimmed and sealed with a CRA weld overlay, so the joint between liner and host is closed before the pipe leaves the mill.

Metallurgically clad pipe has no separate liner at any stage. There are two main routes. In the plate route, CRA and carbon steel plates are joined first, by hot roll bonding or by explosion bonding, then the explosion bonded clad plates are formed by JCOE or UOE and seam-welded, with the inside seam finished in CRA weld metal. This is how our explosion welding pipe is produced. In the overlay route, CRA is deposited directly onto the bore of a seamless or welded pipe by hot-wire GTAW or strip cladding. That route gives weld overlay pipes with clad ID, and the critical variable is iron dilution: specifications commonly cap iron in the finished Alloy 625 surface at 5 or 10 percent, which is why two or more layers are often applied. A third option, centrifugally cast or co-extruded bimetallic pipe, is seen less often in line pipe sizes.

Because the products hold together differently, the QA plans measure different things.

For clad pipe, the interface is a weld-like joint and is tested like one. Shear tests on production coupons confirm bond strength; ASTM A264 and A265 set the familiar 140 MPa (20 ksi) minimum for clad plate, and API 5LD carries a shear requirement for the finished pipe. Guided bend tests show whether the layer stays attached when strained. Full-body ultrasonic scanning, with ASTM A578 as the usual reference for plate, maps any unbonded areas, and PMI or chemical analysis on the CRA surface checks alloy and dilution.

For MLP there is no bond to shear, so the tests look at the grip and the seal. The mill measures gripping force or residual contact pressure on rings cut from production pipe, checks the liner for wrinkles and local collapse, and verifies ovality. The end-seal overlays get dye penetrant and dimensional checks, and many owners now add a helium leak test on the annulus to catch pinholes that a visual inspection would never find. The weakest point of a lined pipe is its end seal, so this is where an inspector’s time is best spent.

One practical tip: agree the sampling frequency before production starts. API 5LD and most owner specifications define tests per heat or per lot, but a “lot” means different things for clad plate, finished pipe and overlay batches. Settling it at the pre-production meeting, together with the tests the third-party inspector will witness, saves days of argument when the first release note is due.

ItemMechanically Lined PipeMetallurgically Clad Pipe
Starting materialOuter line pipe plus a separate CRA liner tubeRoll- or explosion-bonded plate, or pipe with internal overlay
How the layers joinHydraulic or mechanical expansion, interference fitBonding before forming, or fusion during overlay welding
Key interface testGripping force / contact pressure, liner wrinkle checkShear test, bend test, 100% UT for unbonded areas
Pipe endsCRA overlay seal applied at the millCRA continuous to the bevel
Extra checksAnnulus helium leak test, end-seal PTIron dilution on overlay, CRA thickness mapping
Typical lead time quotedShorter, often 6 to 10 weeksLonger, often 12 to 20 weeks
Temperature range often citedModerate, frequently held below about 150 to 200 °CConsiderably higher, up to around 400 °C for bonded pipe

Lead times and temperature limits vary from mill to mill and project to project, so treat these figures as starting points for a technical query, not as acceptance values.

A common assumption is that clad pipe is lighter because the CRA layer “adds strength”. In most designs it does not. Under ASME B31.3 for plant piping, and in normal pipeline practice, the CRA layer is excluded from the pressure-containing wall and treated as a corrosion barrier. The backing steel alone must satisfy the wall thickness calculation. So for the same design pressure, a clad pipe and a lined pipe end up with essentially the same carbon steel wall and very similar weight.

The second misreading concerns CRA thickness. A figure of 3.0 mm minimum appears in most owner specifications, but buyers sometimes quote it as nominal. On overlay pipe, nominal thickness after machining can easily drop below the minimum near the ends. Always state the CRA thickness as a minimum and say where it is measured.

The third concerns qualification. Welding procedures for clad pipe, including any overlay, are qualified to ASME Section IX for plant work or to the pipeline code for the project. For MLP, the end-seal overlay is a separate qualified procedure, and it should be listed in the ITP with its own hold point.

Much of the 2026 enquiry flow for bimetallic pipe comes from outside traditional sour oil and gas. Carbon capture projects are a good example. Dry, clean CO2 barely corrodes carbon steel, but once free water and impurities such as oxygen, SOx or NOx are present, the stream can become strongly acidic. Many CCS designers therefore specify a CRA barrier in the sections most likely to see wet CO2, such as compression outlets, injection wells and offshore risers. These lines also undergo planned and emergency depressurization, and dense-phase CO2 cools sharply as it expands. Low temperature and rapid pressure drop are exactly the conditions where a bonded layer is the safer choice, and where the backing steel needs Charpy toughness proven at low temperature.

Seawater injection is the opposite case. Flow is steady, temperature is close to ambient, and the lines are long and straight, which makes MLP a reasonable candidate. The alloy matters more than the bond here: 316L is not a safe choice in oxygenated seawater, so Alloy 625 or super duplex is usually specified.

For hydrogen and hydrogen blends, the CRA layer is rarely the governing issue. Attention falls on the backing steel and the girth welds, and owners are qualifying those lines case by case. Ask your supplier for test data on the backing grade before committing to either product.

A clear RFQ removes most of the arguments at the inspection stage. We recommend stating:

  • Product type per API 5LD (clad or lined), and whether the alternative is acceptable.
  • Backing grade and PSL, for example ISO 3183 L450QS / X65QS PSL 2, with any sour or offshore annex.
  • CRA alloy and minimum thickness, and the iron dilution limit if overlay is permitted.
  • Interface tests, sampling frequency and acceptance values for shear, bend, gripping force or leak testing.
  • End preparation: bevel geometry, CRA overlay length for lined pipe, and machining tolerances.
  • Hydrotest, NDT coverage, EN 10204 3.1 or 3.2 certificates and third-party inspection.
  • Packing: end caps, nylon slings, no contact with carbon steel tools, and chloride-free protection for sea freight.
  • Matching bends, fittings and flanges, ordered with the pipe so that alloy and bevel details line up.

Our mill produces CRA clad pipe for sour service and offshore by explosion bonding, roll bonding and internal weld overlay. Typical orders include SS316/316L explosion bonded clad pipe on API 5L backing and Incoloy 825 clad line pipe in L450QS / X65QS PSL 2 for sour gas. Because a pipeline is more than straight pipe, we also manufacture CRA clad pipe fittings, clad and overlay flanges and clad induction bends, so one ITP and one set of documents can cover the whole package. The full product family is listed under CRA Clad & Weld Overlay Piping.

In clad pipe the CRA and the steel are joined by a metallurgical bond made by roll bonding, explosion bonding or weld overlay. In MLP a separate CRA liner is held inside the steel pipe by interference from expansion. Both are covered by API 5LD.

Normally not. The backing steel is designed to carry the full pressure, and the CRA layer is treated as a corrosion barrier, for both clad and lined pipe.

For clad pipe: shear and bend tests on production samples plus full-body UT for unbonded areas. For MLP: gripping force or contact pressure tests, liner wrinkle checks and leak testing of the end seals.

MLP is usually quicker because both components are standard products. Clad pipe takes longer, especially when bonded plate must be produced first. Fittings and bends often set the critical path for either product.

It can be used in steady, well-dried sections, but many designers prefer clad pipe where wet CO2, frequent depressurization or low temperatures during blowdown are expected.

Yes. The lined pipe end overlay and the clad pipe CRA layer are joined with a nickel-alloy girth weld under a qualified procedure. Clad fittings and bends are routinely installed in lined pipelines.

316L suits mild chloride service, Alloy 825 is common for sour gas and acidic conditions, and Alloy 625 is used for higher chlorides, seawater and severe sour duty. Final selection should follow NACE MR0175 / ISO 15156 and the corrosion study.

Fit end caps or bevel protectors, lift with nylon slings, keep the CRA bore away from carbon steel tools and wire ropes, and protect against salt spray during sea freight. Iron contamination on the bore can start pitting before the line is ever commissioned.

Planning a clad or lined pipeline? Send us your line list, service conditions, backing grade and CRA alloy through the inquiry form on petrolsteel.com. Our engineering team will review the specification and return a technical clarification list with the quotation.

INQUIRY US

Related News

Product Categories

Need a Quote?

Send OD, WT, grade & quantity — get ex-factory pricing within 24 hrs.